HOEYWELL SECTION II – CLEANING 3. Standard Cleaning Methods 标准清洁方法

3. Standard Cleaning Methods 标准清洁方法 CAUTION: SPECIFIED CLEANING METHODS OUTLINED MUST BE FOLLOWED. THE VARIOUS SOLUTIONS AND MATERIALS SPECIFIED IN THE CLEANING METHODS CAN B...
SOPM20-11-08如何编程可编程电路设备-航修札记

SOPM20-11-08如何编程可编程电路设备

如何编程可编程电路设备HOW TO PROGRAM PROGRAMMABLE CIRCUIT DEVICES 1. INTRODUCTION 介绍 A. The data in this subject gives general procedures to put programs into Boeing-supplied pro...
3月5日
0130
SECTION IV – REPAIR 14-零件重新标记-航修札记

SECTION IV – REPAIR 14-零件重新标记

14. Remarking Parts 零件重新标记Before to start cleaning, locate the marks that can be removed by the cleaning and repainting process. Those marks must be identified and recorded. ...
SECTION IV – REPAIR 2.溶液制备-航修札记

SECTION IV – REPAIR 2.溶液制备

2.Preparation of Solutions溶液制备WARNING: SOLUTIONS USED FOR CLEANING ARE HAZARDOUS. AVOID INHALING FUMES, DUST, OR MIST. AVOID CONTACT WITH SKIN. AFTER PREPARATION, WASH HANDS AN...
SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-K.Method No. 403K:修复受损的油漆涂层-环氧胺体系-航修札记

SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-K.Method No. 403K:修复受损的油漆涂层-环氧胺体系

3. Repair and Application of Protective Coatings and Plating 防护涂料及电镀的修复与应用K.Method No. 403K: Repair of Damaged Paint Coatings - Epoxy-Amine SystemsMethod No. 403K:修复...
SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-E.Method No. 403E:干膜润滑剂修复-航修札记

SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-E.Method No. 403E:干膜润滑剂修复

3. Repair and Application of Protective Coatings and Plating 防护涂料及电镀的修复与应用E.Method No. 403E: Dry-film Lubricant RepairMethod No. 403E:干膜润滑剂修复Dry-film lubricant...
SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-A.Method No. 403A: 阳极氧化铝和铝合金修复-航修札记

SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-A.Method No. 403A: 阳极氧化铝和铝合金修复

3. Repair and Application of Protective Coatings and Plating 防护涂料及电镀的修复与应用A.Method No. 403A: Anodized Aluminum and Aluminum-alloy RepairMethod No. 403A: 阳极氧化铝和铝...
SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-B.Method No. 403B: 硬铬镀件修复-航修札记

SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-B.Method No. 403B: 硬铬镀件修复

3. Repair and Application of Protective Coatings and Plating 防护涂料及电镀的修复与应用B.Method No. 403B: Hard Chrome Plated Parts RepairMethod No. 403B: 硬铬镀件修复NOTE: Hard chr...
SOPM20-50-15浇铸非金属垫片的安装-航修札记

SOPM20-50-15浇铸非金属垫片的安装

浇铸非金属垫片的安装INSTALLATION OF CASTABLE NON-METAL SHIMS 1. INTRODUCTION 介绍 A. This data in this subject comes from Boeing Process Document D042T613. The airline has or can g...
3月30日
0110
SECTION IV – REPAIR 5.清除钢制零件上的损伤-B.Method No. 405B:去除严重腐蚀、硬碳、油漆和氧化皮-航修札记

SECTION IV – REPAIR 5.清除钢制零件上的损伤-B.Method No. 405B:去除严重腐蚀、硬碳、油漆和氧化皮

5.Removing Damage from Steel Parts清除钢制零件上的损伤B.Method No. 405B: Heavy Corrosion, Hard Carbon, Paint, and Scale RemovalMethod No. 405B:去除严重腐蚀、硬碳、油漆和氧化皮Remov...
SECTION III – INSPECTION 1. Standard Inspection Practices -M.用于电子设备校准和检查的热电偶模拟器-航修札记

SECTION III – INSPECTION 1. Standard Inspection Practices -M.用于电子设备校准和检查的热电偶模拟器

M.Thermocouple Simulators for Calibration and Checkout of Electronic Equipment 用于电子设备校准和检查的热电偶模拟器(1) For test purposes in simulating a thermocouple, a common and ...
SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-G.Method No. 403G:耐磨涂层表面磨损修复-航修札记

SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-G.Method No. 403G:耐磨涂层表面磨损修复

3. Repair and Application of Protective Coatings and Plating 防护涂料及电镀的修复与应用G.Method No. 403G: Abradable Coating Surface Wear RepairMethod No. 403G:耐磨涂层表面磨损修复N...
SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-F.Method No. 403F:等离子喷涂修复-航修札记

SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-F.Method No. 403F:等离子喷涂修复

3. Repair and Application of Protective Coatings and Plating 防护涂料及电镀的修复与应用F.Method No. 403F: Plasma Spray RepairMethod No. 403F:等离子喷涂修复NOTE: Electric Arc Metal...
SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-I.Method No. 403I:化学镀镍-航修札记

SECTION IV – REPAIR 3. 防护涂料及电镀的修复与应用-I.Method No. 403I:化学镀镍

3. Repair and Application of Protective Coatings and Plating 防护涂料及电镀的修复与应用I.Method No. 403I: Electroless Nickel PlatingMethod No. 403I:化学镀镍CAUTION: BECAUSE OF MASK...
SECTION IV – REPAIR 4. 修理铝制零件-B.Method No. 404B: 去除严重腐蚀、硬质碳、油漆和水垢-航修札记

SECTION IV – REPAIR 4. 修理铝制零件-B.Method No. 404B: 去除严重腐蚀、硬质碳、油漆和水垢

4. Repairing Aluminum Parts 修理铝制零件B.Method No. 404B: Heavy Corrosion, Hard Carbon, Paint, and Scale RemovalMethod No. 404B:去除严重腐蚀、硬质碳、油漆和水垢Remove heavy corros...
SECTION IV – REPAIR 4. 修理铝制零件-C.Method No. 404C:沟槽和划痕修复-航修札记

SECTION IV – REPAIR 4. 修理铝制零件-C.Method No. 404C:沟槽和划痕修复

4. Repairing Aluminum Parts 修理铝制零件C.Method No. 404C: Gouge and Scoring RepairMethod No. 404C:沟槽和划痕修复Repair gouges, scoring, etc., on aluminum-alloy parts as follows:按...
SECTION IV – REPAIR 4.修理铝制零件-A.Method No. 404A:轻微表面缺陷修复-航修札记

SECTION IV – REPAIR 4.修理铝制零件-A.Method No. 404A:轻微表面缺陷修复

4.Repairing Aluminum Parts修理铝制零件A.Method No. 404A: Minor Surface Defect RepairMethod No. 404A:轻微表面缺陷修复Repair minor surface defects on aluminum-alloy parts as follows:...